MIM F1537 (ASTM F1537) HIP and Heat Treat
Material Properties ASTM F1537 Kinetics
Hot-Worked Annealed Typical
Ultimate Strength (KSI) 145 130 160
Yield Strength (KSI) 101 75 85
Elongation (% in 1") 12 20 27
Reduction in Area (%) - - 23
Surface Finish (Ra) - - 40
Impact Energy (ft-lbf)1 - - 80
Macro Hardness (RC) - - 32
Sintered Density (g/cm3) - - 8.27 (HIP)

1Test method uses 1/2 sized un-notched charpy bar.

 

Material Description:
Most Commonly used in the medical market on applications requiring these characteristics:

  • Bio-compatibility
  • Corrosion resistance
  • High strength
  • Nonmagnetic
  • Wear resistance

 
Material Composition (%):
 
Co Ni (Max) Cr Mo C Mn (Max) Si (Max) N (Max) Fe (Max)
Balance 1 26-30 5-7 0.1-0.35 1 1 0.25 .75

 
Click Here to Print This Page

 
About Our Company | Metal Injection Molding | Application Review | Request a Quote | Materials & Properties | What's New | Employment Opportunities | Contact Us | File Transfers | MIM Design Guide | Ask a PIM/MIM Expert a Question | Climax Engineered Materials | Home

Copyright © 2003 Kinetics. All Rights Reserved. Site designed and hosted by The Worx Group. Email the webmaster.